第44卷第1期
2016年1月【科研与生产】
聚氯乙烯 Polyvinyl Chloride
干燥工艺对PVC树脂质量的影响
赵丽颖·
(唐山三友氯碱有限责任公司,河北唐山063305)
【关键词】PVC;旋风干燥器;杂质粒子数;挥发物质量分数;影响因素;措施
Vol.44,No.1 Jan.,2016
[摘要】针对PVC树脂在旋风干煤过程中容易出现杂质粒子数、挥发物质量分数超标的间题,进行了原因分析,并提出了解决措施:①干燥过程中实时监控产品性能,②及时隔离不合格树脂,③定期清理干燥系统,④定期更换空气过滤棉。
【中图分类号】TQ325.3
【文献标志码]B
0
Effect of drying process on the quality of PVC resins
ZHAO Liying
(Tangshan Sanyou Chlor Alkali Co., Ltd., Tangshan 063305,China)
Key words: PVC; cyclone dryer; impurity particle number; volatile matter mass fraction; influen-
cingfactor;measure
Abstract: In order to solve the problem that impurity particle number and volatile matter mass frac-tion of PVC resin were sub-standard in cyclone drying process, reasons were analyzed, and improvement oa process, (2) in time separating unqualified PVC resin from qualified PVC resin, (3) regularly cleaning dr-ying system, (4)regularly replacing air filter cotton
悬浮法PVC树脂产品国家标准中,共规定了 10项检测指标,即黏数、杂质粒子数、挥发物质量分数、表观密度、筛余物、“鱼眼”数、增塑剂吸收量、白度、水萃取液电导率和残留氯乙烯含量。通过对 PVC树脂各项性能的统计分析,发现杂质粒子数和挥发物质量分数超标是影响唐山三友氟碱有限责任公司PVC树脂产品等级的主要原因,而这两项指标的控制主要集中在干燥工序,因而干燥工序的控制情况直接影响树脂成品的优等品率。
旋风干燥工艺流程 1
经离心机脱水后得到的滤饼由螺旋输送器送人干燥筒气流管下部,与从换热器来的150℃左右的热空气接触,树脂表面的水分被带走,热空气的温度
,【收稿日期】201508-13
也迅速下降,树脂与降温后的热空气由干燥简气流管顶部送出后沿切线进人旋风干燥器底部。
在旋风干燥器内,树脂与热空气旋转而上,进一步干燥后由干燥器上部沿切线送出。空气经过滤器过滤后,用鼓风机增压,再经空气加热器进人干燥筒气流管的底部吹送和干燥物料。干燥好的物料和再次降温的热空气由抽风机抽至旋风分离器,使气固相分离,尾气再经进一步气固分离后排空,从旋风分离器底部下来的物料经过振动筛筛分后,进人料仓")。
旋风干燥工艺流程见图1。
【作者简介】赵丽额(1982一),女,工程师,2005年毕业于燕山大学应用化学专业,现从事PVC树脂及糊树脂的生产研发
工作。 14
万方数据