18
doi:10.3969/i. issn. 1009 3230.2012.08.006
应用能源技术
2012年第8期(总第176期)
炉管内聚合物结垢规律测试研究
杨敬彪”,郑海珠,宫克勤
(1.大庆油田装备制造集团,黑龙江大庆163411;2.大庆油田电力集团,黑龙江大庆163453;
3.东北石油大学土木建筑工程学院,黑龙江大庆163318)
摘要:建立了管内聚合物结垢热阻测试试验台。采用对比法对管内聚合物热阻进行了测试研究,分析聚合物结垢的影响因素。测试结果表明:聚合物浓度越高,聚合物结垢层越厚,热阻也越大;随着混合液温度的升高,管内聚合物垢层及热阻都呈现逐步增大的趋势;随着管内聚合物溶液流速的提高,聚合物热阻下降。
关键词:聚合物;结垢热阻;测试中图分类号:TE08
文章编号:1009-3230(2012)08001803
文献标志码:A
TestonthePolymerFoulingLawintheFurnaceTube
YANG Jing-biao', ZHENG Hai-zhu’, GONC Ke-qin
(1.DaqingOilfieldEquipmentManufacturingGroup,Daqing163411,China;
2.Daqing Oilfield Power Group,Daqing 163453, China;
3.Civil Engineering College,Northeast Petroleum University,Daqing 163318,China)
Abstract: The testing device of polymer fouling thermal resistance is established firstly, and the polymer thermal resistances inside the tube were tested by contrast method. The test results indicate that: the higher the polymer concentration, fouling layer is thick, and the thermal resistance is greater; with the increasing of mixed liquid temperature, polymer fouling layer and thermal resistance increase gradually; while the polymer resistance drops with the solution velocity increasing inside the tube.
Key words: Polymer; Fouling thermal resistance; Testing
0引言
油田采用聚合物驱油技术时,采出液中常含有大量聚合物残留。含有聚合物的采出液在通过水套加热炉加热的过程中,混合溶液由于受热而黏度增大,形成具有很高黏弹性的凝胶状混合物,极易与水中的原油及杂质形成黏团状物质并在炉管内壁堆积下来,形成特殊的聚合物结垢层,不仅使炉管传热热阻增大,降低换热管的传热能力,同时使得管内流动阻力增大,甚至堵塞通道。
收稿日期:20120511修订日期:20120607
作者简介:杨敏彪(1969-),男,工程师,主要从事热能工程
方向研究。
万方数据
文中通过建立聚合物热阻测试试验台,测试不同结垢条件下的聚合物垢层热阻,从而研究管内聚合物浓度、介质温度,以及聚合物混合液流速对聚合物结垢过程的影响,探讨聚合物结垢过程的规律。
1对比法传热管垢层热阻测试原理 1.1传热方程
根据传热学原理,被加热介质通过炉管壁所传递的热量Q:
Q=KFAt
(1)
式中:F传热管的传热面积;K--传热系数; △t-传热温差。