一次摊圆封头质量事故的分析
李晓瘾,孙勇,宋烤
(中航黎明锦西化工机械(集团)有限责任公司,辽宁葫芦岛125001)
【关键词】封头;外径;内径;模具;冲压;工艺流程
Vol.42,No.3 Mar.,2014
【摘要】介绍了EHB椭圆封头的冲压工艺流程以及生产中出现的一次质量事故,发现事故原因为操作人员将EHA模具误认为EHB模具用于圆封头的生产。相同直径的EHA与EHB模具的曲面高度不同,因此不能混滑使用。
【中图分类号】TQ340.63;TQ325.3
[文献标志码】B
[文章编号]10097937(2014)03003704
Analysis of an elliptical head quality accident
LIXiaowei,SUNYong,SONGJun
(AVIC Liming Jinxi Chemical Mechinery(Group)Co.,Ltd.,Huludao 125001,China) Key words: head; external diameter; internal diameter; mould; stamping; process flow
Abstract;The stamping process of EHB elliptical head and a quality accident occured in production were introduced. It was found that the cause of the accident was that the operator mistook the EHA mould for EHB mould in the elliptical head production. The EHA mould and EHB mould of the same diameter had different curved surface height, so they could not be misused.
封头的应用非常广泛,因此国家对封头质量非常重视,GB/T25198—2010《压力容器封头》对封头尺寸、材质等有详细的规定,对封头制造厂家提出了强硬的质量要求。封头的种类繁多,按用途可分为承压封头和常压封头,按形状可分椭圆封头、蝶形封头、球罐形封头、半球形封头、弓形封头、平底形封头、锥形封头等。由于椭圆封头受力较好,加工较容易,其广泛应用于聚合釜和压力容器中。椭圆封头的质量不但直接影响产品质量和成本,而且还影响生产装置的安全、长期运行。根据直径的划分基准,椭圆封头可分为EHA(以内径为基准)和EHB(以外径为基准)2种")。中航黎明锦西化工机械(集团)有限责任公司在生产PVC聚合釜的EHB椭圆封头过程中出现了质量间题,笔者对其进行了分析。
【收稿日期】2013-12-25
1EHB椭圆封头简介
该EHB椭圆封头的外径为(508±1.5)mm,最小壁厚为30mm,材质为S32168。考虑到热压过程中坏料的收缩,将坏料厚度增加到34mm(具体计算过程见后文)。GB/T25198—2010中规定:当封头公称直径≤2000mm时,直边长度(h)为25mm,公差为-5%~10%。EHB椭圆封头及增口坡口的加工图如图1所示。
34
508
(a)桶圆封头
【作者简介】李晓巍(1982一),女,助理工程师,2004年毕业于沈阳化工大学,现于中航黎明锦西化工机械(集团)有限
责任公司从事机械设计方面的工作。