70m3聚合釜的防粘釜及清釜技术改良
梁云龙“
(四平昊华化工有限公司,吉林四平136001)
[关键词]PVC;70m’聚合签;粘签;防粘签技术;雾化;清签技术
Vol. 39, No. 10
Oct.,2011
[摘要]通过研究聚合釜粘签的主要原因和防粘签技术,改良了涂签的雾化方法和清签技术。改进后聚合签运行正常,降低了防粘釜剂和纯水的用量,缩短了清釜周期,提高了PVC树脂产品的产量和质量,年净增效益可达 29万元。
[中图分类号]TQ325.3;TQ320.6
[文献标志码]B
[文章编号】1009-7937(2011)10-0037-03
Modification on antiscaling and cleaning technologies for 70m’polymerizers
LIANG Yunlong
(Siping Haohua Chcmical Industry Co., Ltd., Siping 136001, China)
Key words;PVC; 70 m polymerizer; polymcrizer scaling; antiscaling technology; spraying; polymerizer cleaning technology
Abstract: Based on rescarch on reasons for polymcrizer scaling and thc antiscaling tcchnologies, mcthods for spraying coating polymcrizer were modified as well as thc polymcrizcr clcaning mcth-ods.After improvemcnt,the polymcrizcrs ran stcady, the consumption amount of antisacling agcnts and water were lowered, the polymerizer clcaning periods were shortened, the output and quality of PVC resins wcre improved, and thus the nct bcnefit could increase by O.29 million RMB Y per ycar.
PVC工业化生产以来,无论是悬浮法、乳液法还是本体法工艺,都会遇到聚合物粘结于釜壁、搅拌桨叶以及釜上气相管道的所谓粘釜问题。粘釜会导致聚合釜传热系数和生产能力下降;粘釜料者混人产品中,会产生塑化加工时的暂时或永久的“鱼眼”,影响制品的外观和内在质量;粘釜物的清理将延长聚合签的辅助生产时间,降低设备运转率,此外,粘釜还影响到聚合釜自动控制的实施。这诸多弊端,
都会直接或间接地影响经济效益。 1
粘釜的主要成因
通过对粘釜影响因素、粘签粒子的观察以及大量的防粘釜技术研究,发现粘釜的形成机制可归结于以下两种因素。
(1)物理因素。
物理吸附粘釜主要是由于釜壁光洁度差而使粘釜加重。不锈钢釜由于加工光洁度不高造成釜壁粗糙,
,[收稿日期]2011-01-17
以及釜壁受到机械损伤和聚合反应过程中HCI对釜壁产生的腐蚀等因素,造成氯乙烯进入聚合釜后吸附在钢表面能量较高处,故聚合物易于在此处吸附形成粘签中心,并在这些中心进一步聚合而使粘釜加重。当聚合转化率在10%~30%时,颗粒外层的“皮膜”尚未成熟,内部呈黏稠状态,此时若机械因素使颗粒撞破“皮膜”,流出的黏稠物则易与釜壁或搅拌轴黏附而形成粘釜中心。上述粘釜是由于物理吸附而无化学键存在,所以与釜壁的结合力较弱,比较容易清除。
(2)化学因素。
化学粘釜包括化学键粘釜、配合粘釜及二、三次粒子粘釜、水相聚合粘釜。其中主要是化学键粘釜、水相聚合粘签。与电子自由基催化理论相似,假定不锈钢表面各晶格的结点之间,由于温度等外界条件的能量激发,存在着一些移动的和平衡的自由电子和相应的失去电子的孔穴,它们犹如通常的原子
[作者简介]梁云龙(1983一),助理工程师,毕业于吉林化工学院高分子材料与工程专业,于四平昊华化工有限公司从
事聚氯乙烯的生产管理工作。
37