总第260期 2017年第8期
河北冶金 HEBEI METALLURGY
热轧平整机组平整花纹板的方法
白君,高茂林,杨海峰
(河钢集团承钢公司板带事业部,河北承德067002)
Total No. 260 2017,Number8
摘要:针对薄规格热轧板存在的浪形间题,从“机、电、液”相融合的角度出发,对热轧平整机组作机械设备选型,提高平整机压下和零调的精度,避免花纹板豆高的影响:调节加速斜坡控制参数,减小加速度,使得加速过程变得平稳:结合HGC压下系统工作原理,在电气控制程序中增加压力反馈值平滑滤波处理优化PI调节器参数,抑制振动干扰。采用多种轧辑辊形的经验曲线,配合平整机弯辑减少热轧板表
面浪形。经生产验证,热轧平整机组平整花纹板效果良好。关键词:热轧平整机组:花纹板;方法
中图分类号:TG333.4
文献标识码:B
doi : 10. 13630/j. cnki. 13 1172. 2017. 0814
文章编号:10065008(2017)08004903
METHODTOTEMPERCHECKERDE
PLATEINHOT-ROLLINGTEMPERMILL
Bai Jun,Gao Maolin,YangHaifeng
( Board Strip Department, HBIS Group Chengsteel Company, Chengde, HeBei, 067002)
aeaoaaoe machine, electricity, liquid" , the machinery equipment is selected for the hot rolled lemper mill, the screw aaraoaearaaaeaeeao tion process becomes stable by adjusting acceleration ramp control parameters and reducing the acceleration; the pressure feedback value smoothing and filtering treat is added into the electric contral program to aptimige the PI regulator parameters to suppress vibration interference, combining with the working mechanism of HGC pressure system. A variety of roll shape experience curve is adopted, and combined with the bending roll of the temper mill, the surface wave of hot rolled plate is reduced. The test results show that the check-
ered plate flattening of hot rolling temper set has good effect. Key Words : hot rolling temper mill; checkered plate; method
0
引言
目前.热轧卷板生产线下线的薄规格花纹板板
形问题较为突出,3mm厚度花纹板不平度达到了 14mm/2m。由于下游客户的需求和热轧花纹板产品的开发,热轧卷板生产线的花纹板厚度逐步减薄,花纹板板形质量异议较多,影响了产线效益。国内热轧平整机组只通过矫直模式对带有浪形的花纹板进行处理,板形质量达不到用户的要求。因此,提出了采用平整模式对花纹板进行处理,提高薄规格花
纹板的成材率。收稿日期;2017-04-11
作者简介:白君(1982-),男,工程师,2013年毕业于河北联合大学材料成型与控制工程专业,现在河钢集团承钢公司板带事业部从事热轧带钢研究与生产工作,E-mail;378642342@qq-com
万方数据
1
技术方案
热轧平整机组平整花纹板技术方案的实施主要包括机械、电气、轧辊三个方面。机械方面涉及平整机HGC液压缸选型、轧制线调整装置选型;电气方面涉及传动控制系统速度斜坡参数优化、HGC压下控制系统PI调节器和比例系数优化、压力传感器反馈值加滤波处理:工作辑改变原来单一的sne负凸
度或多次方负凸度辊形,使用经验曲线。 1.1
机械设备选型
(1)优化平整机HGC液压缸缸体的加工技术指标,提高轧制精度。
(2)选用斜楔+液压缸+位置传感器的轧制线调整方式,有助于引人花纹板豆高的调零方式。
49